OSB, no insulation, rep 2

Oriented Strand Board (OSB)

Description

This experiment is on a system consisting of an Oriented Strand Board (OSB) cladding panel alone, with no insulation panel. It is the second repetition of this system configuration.

Experiment Notes

At approximately 11 minutes the OSB panel began to collapse, causing a sudden change in the mass measurements as debris fell into the debris tray, onto both load cells, or off the entire assembly.

Test Details
Cladding Oriented Strand Board (OSB)
Cladding Thickness [mm] 11
Insulation No insulation
Insulation thickness [mm]
Cavity width [mm]
Repetition number 2
Metrics
Peak HRR [kW] 123
Time to Peak HRR [mins] 10.33
Total HR [MJ] 48.3
Peak dQ/dt [kW/s] 0.468
Time to Peak dQ/dt [mins] 9.23
Residual HRR [kW] 8.5
Test Pictures (click to zoom)
Download Data (CSV) Download Data (PDF)
Video
HRR [kW] including burner baseline
Minutes
30