OSB, no insulation, rep 3

Oriented Strand Board (OSB)

Description

This experiment is on a system consisting of an Oriented Strand Board (OSB) cladding panel alone, with no insulation panel. It is the third repetition of this system configuration.

Experiment Notes

At approximately 10 minutes the OSB panel began to collapse, causing a sudden change in the mass measurements as debris fell into the debris tray, onto both load cells, or off the entire assembly.

Test Details
Cladding Oriented Strand Board (OSB)
Cladding Thickness [mm] 11
Insulation No insulation
Insulation thickness [mm]
Cavity width [mm]
Repetition number 3
Metrics
Peak HRR [kW] 118
Time to Peak HRR [mins] 9.48
Total HR [MJ] 44.5
Peak dQ/dt [kW/s] 0.612
Time to Peak dQ/dt [mins] 9.53
Residual HRR [kW] 6.26